Material GuideSpring Materials We Use
Typical values — tensile strength depends on wire size. Our engineers confirm the right grade for your load, temperature and environment.
Carbon spring steel wire
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| IS 4454-1 Grade SL / SM / SH | IS 4454-1 / EN 10270-1 | 79,500 | 1,200 – 2,230 | 120 | Static springs, general purpose |
| IS 4454-1 Grade DM / DH | IS 4454-1 / EN 10270-1 | 79,500 | 1,400 – 2,230 | 120 | Dynamic springs, automotive, machinery |
| ASTM A228 Music Wire | ASTM A228 | 81,500 | 1,590 – 2,750 | 120 | Small high-stress precision springs |
| ASTM A229 Oil-tempered | ASTM A229 | 79,500 | 1,450 – 1,900 | 150 | General oil-tempered springs |
Oil-hardened & alloy steel
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| IS 4454-2 FDC / VDC | IS 4454-2 / EN 10270-2 | 79,500 | 1,600 – 2,000 | 150 | Valve and fatigue-critical springs |
| IS 4454-2 FDCrV / ASTM A232 | EN 10270-2 / ASTM A232 | 79,500 | 1,550 – 1,900 | 220 | Valve springs, shock loads |
| EN 10270-2 VDSiCr / ASTM A401 | EN 10270-2 / ASTM A401 | 79,500 | 1,900 – 2,150 | 250 | High-stress engine valve springs |
| 50CrV4 bar (hot coiled) | EN 10089 | 78,500 | 1,250 – 1,650 | 220 | Heavy-duty railway & industrial springs |
| 65Mn | GB/T 1222 | 78,500 | 1,080 – 1,320 | 150 | Flat springs, washers, clips |
Strip steel
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| SAE 1074 / 1075 (CK75) | EN 10132-4 | — | 1,200 – 1,520 | 120 | Flat springs, clips, wave springs |
| SAE 1095 (CK101) | EN 10132-4 | — | 1,380 – 1,650 | 120 | High-stress flat & wave springs |
| 51CrV4 strip | EN 10132-4 / DIN EN 16983 | 78,500 | 1,250 – 1,600 | 200 | Disc springs (Belleville) |
Stainless steel
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| SS 302 / 304 | EN 10270-3 / ASTM A313 | 69,000 | 1,550 – 2,200 | 300 | Corrosion-resistant general springs |
| SS 316 / 316L | EN 10270-3 / ASTM A313 | 69,000 | 1,380 – 1,930 | 300 | Marine, chemical, food & pharma |
| SS 17-7 PH | EN 10270-3 / ASTM A313 | 75,800 | 1,450 – 2,070 | 370 | High strength stainless, aerospace |
Nickel super-alloys
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| Inconel 718 | AMS 5832 | 79,300 | 1,240 – 1,450 | 700 | High temperature, oil & gas, aerospace |
| Inconel X-750 | AMS 5699 | 79,300 | 1,100 – 1,380 | 650 | High-temperature relaxation resistance |
| Inconel 625 | AMS 5837 | 79,000 | 1,035 – 1,380 | 650 | Corrosive & high-temperature service |
| Hastelloy C-276 | UNS N10276 | 78,600 | 1,300 – 1,700 | 400 | Highly corrosive chemical & sour service |
Non-ferrous & titanium
| Material / Grade | Standard | G (N/mm²) | Rm (N/mm²) | Max °C | Typical use |
|---|
| Phosphor Bronze | ASTM B159 | 41,000 | 550 – 900 | 100 | Electrical contacts, non-magnetic |
| Beryllium Copper | ASTM B197 | 48,000 | 1,100 – 1,380 | 200 | Conductive, non-sparking springs |
| Titanium Ti-6Al-4V | AMS 4928 | 44,000 | 895 – 1,170 | 315 | Lightweight, corrosion-resistant |
G = shear modulus. Rm = tensile strength range (decreases with larger wire diameter). Max °C = typical maximum service temperature. Values are indicative; design is verified to EN 13906 / IS 7906.